FR408HR高速板材規(guī)格參數(shù)

      FR408HR層壓板是采用高性能多功能樹脂和電氣級(E-玻璃)玻璃纖維織物加固壓制而成。該材料在Z軸擴展方面提高了30%,并且提供了比該領(lǐng)域競爭產(chǎn)品多25%的電帶寬(更低的損耗)。這些特性加上在回流焊時優(yōu)越的防潮性,使得產(chǎn)品能夠從熱和電的角度來提高板的優(yōu)質(zhì)性。


PropertyTypical ValueUnitsTest Method
Metric (English)IPC-TM-650 (or as noted)
Glass Transition Temperature (Tg) by DSC190°C2.4.25C
Decomposition Temperature (Td) by TGA @ 5% weight loss360°C2.4.24.6
Time to Delaminate by TMA (Copper removed)

A. T260

B. T288

60

>30

Minutes2.4.24.1
Z-Axis CTE

A. Pre-Tg

B. Post-Tg

C. 50 to 260°C, (Total Expansion)

55

230

2.8

ppm/°C

ppm/°C

%

2.4.24C
X/Y-Axis CTEPre-Tg16ppm/°C2.4.24C
Thermal Conductivity0.4W/mKASTM E1952
Thermal Stress 10 sec @ 288oC (550.4oF)

A. Unetched

B. Etched

PassPass Visual2.4.13.1
Dk, Permittivity

A. @ 100 MHz

B. @ 1 GHz

C. @ 2 GHz

D. @ 5 GHz

E. @ 10 GHz

3.72

3.69

3.68

3.64

3.65

2.5.5.3

2.5.5.9

Bereskin Stripline

Bereskin Stripline

Bereskin Stripline

Df, Loss Tangent

A. @ 100 MHz

B. @ 1 GHz

C. @ 2 GHz

D. @ 5 GHz

E. @ 10 GHz

0.0072

0.0091

0.0092

0.0098

0.0095

2.5.5.3

2.5.5.9

Bereskin Stripline

Bereskin Stripline

Bereskin Stripline

Volume Resistivity

A. After moisture resistance

B. At elevated temperature

4.4 x 107

9.4 x 107

MΩ-cm2.5.17.1
Surface Resistivity

A. After moisture resistance

B. At elevated temperature

2.6 x 106

2.1 x 108

2.5.17.1
Dielectric Breakdown>50kV2.5.6B
Arc Resistance137Seconds2.5.1B
Electric Strength (Laminate & laminated prepreg)70 (1741)kV/mm (V/mil)2.5.6.2A
Comparative Tracking Index (CTI)3 (175-249)Class (Volts)UL 746A
ASTM D3638
Peel Strength

A. Low profile copper foil and very low profile copper foil all copper foil >17 μm [0.669 mil]

B. Standard profile copper

    1. After thermal stress

    2. After process solutions


1.14 (6.5)


0.96 (5.5)

0.90 (5.1)

N/mm (lb/inch)

2.4.8C


2.4.8.2A

2.4.8.3

Flexural Strength

A. Length direction

B. Cross direction

72.5

58.0

ksi2.4.4B
Tensile Strength

A. Length direction

B. Cross direction

54.5

38.7

ksiASTM D3039
Young's Modulus

A. Length direction

B. Cross direction

3695

3315

ksiASTM D790-15e2
Poisson's Ratio

A. Length direction

B. Cross direction

0.137

0.133

ASTM D3039
Moisture Absorption0.061%2.6.2.1A
Flammability (Laminate & laminated prepreg)V-0RatingUL 94
Relative Thermal Index (RTI)130°CUL 796
The data, while believed to be accurate and based on analytical methods considered to be reliable, is for information purposes only. Any sales of these products will be governed by 

 